Latest company news about How to Produce High Quality Food Grade PVC Cling Film from our PVC Cling Film Machine
November 23, 2026

How to Produce High Quality Food Grade PVC Cling Film from our PVC Cling Film Machine

News Details

High-quality PVC cling film relies on four integrated factors: food-grade formulation, stable film-forming process, precise temperature & tension control, and online quality inspection. It is not determined by a single machine. The following outlines the full industrial production workflow, including how to coordinate with your PVC cling film rewinding & slitting machine.

 

1. Formulation Design (Determines the Quality Ceiling)

1) PVC Powder   64.6%

2) Plasticizer(DOA)  24%

3) Soybean Oil(ESO)  9%

4) Stabilizer         1.2%

5) Anti-fogging      1.2%

Remark: Above Ratio just for your reference, the ration will be a little difference depend on the weather and quality difference.

 

PVC cling film is a soft PVC product. The plasticizer system defines key properties: hand feel, self-adhesion, transparency, odor, and migration level.

 

Reference Formulation (Food-Grade, Parts by Weight)

 

PVC resin: SG-4 / SG-5 (K-value 62–65, low impurities) — 100

 

Primary plasticizer: DOTP 50–65 or DINP / ATBC (prefer DOTP/ATBC for EU/US exports; minimize DOP)

 

Auxiliary plasticizer/stabilizer: Epoxidized,Soybean Oil (ESO) 5–10

 

Heat stabilizer: Ca-Zn composite 2–4 (food-grade; organic tin available for high clarity, subject to local regulations)

 

Anti-fog agent: Food-grade anti-fog agent 0.5–2 (prevents fogging in refrigerated display)

 

Lubricants: GMS / Stearic acid / PE wax — total 1–1.5 (excess causes blooming and haze)

 

Processing aid: ACR 1–2 (improves melt strength, reduces shark skin)

 

Self-adhesion control: Achieved via plasticizer migration rate and surface energy. Avoid paraffin-type additives, which reduce adhesion and increase haze.

 

Red lines: Lead-based stabilizers are strictly prohibited for food contact films. VCM residue ≤ 1 mg/kg. Migration tests must comply with target market standards (e.g., GB 4806.7, EU 10/2011).

 

2. Mixing (Where Many Batch Problems Originate)

 

1) High-speed mixer: Add PVC powder and stabilizer first, then spray plasticizer. Mix at 1000 r/min until 110–120°C to complete pre-plasticization.

 

2) Cooling mixer: Cool down to ≤45°C before discharge to prevent caking and premature decomposition.

 

3) Moisture content: Control ≤0.02%; otherwise bubbles and pinholes will appear in the film bubble.

 

3. Film-Forming Process (Two Options)

 

Option A: Blown Film (Preferred for High-End Export, Low Odor, Uniform Thickness)

 

Barrel temperature: Feed zone 150–160°C / Plasticizing zone 160–170°C / Metering zone 170–180°C

 

Die temperature: 175–185°C; die gap 0.4–1.0 mm

 

Blow-up ratio: 2.5–3.5; take-up speed 30–50 m/min

 

Air ring: Multi-stage air cooling (primary rapid cooling to suppress crystallization; secondary to relieve internal stress; tertiary for sizing)

 

Advantages: No oily feel, high transparency, suitable for thin gauges (6–15 μm)

 

Option B: Calendering (Mainstream for Household Boxed Film, High Output)

 

Roll temperature: 180–200°C; roll gaps gradually reduced to target thickness

 

Thickness tolerance: ±2 μm (on high-end lines)

 

Drawback: Slightly oily feel if excessive plasticizer is used; migration must be controlled via formulation

 

If you purchase jumbo rolls for rewinding: Focus on jumbo roll quality — check thickness CV value, haze, adhesion (N/25mm), odor, and pinholes.

 

4. Cooling & Winding (Determines Roll Appearance and Unwinding Performance)

 

Cooling roll temperature difference: ≤2°C (prevents edge curl and crescent wrinkles)

 

Winding: Closed-loop constant tension control; tension fluctuation ≤ ±0.5 N as roll diameter increases from 200 mm to 800 mm

 

Ionized air static elimination before winding (reduce static from ±5 kV to ≤ ±0.5 kV) to minimize dust attraction

 

If interlayer adhesion is too strong (blocking): Apply food-grade silicone oil release agent 0.3–0.5 g/m²; it volatilizes within 24 hours without affecting use

 

5. Interface Control with Rewinding & Slitting Machine

 

Before the jumbo roll enters the rewinder, the following must be stabilized; otherwise, slit rolls will have uneven edges, loose winding, or telescoping:

 

Jumbo roll edge alignment ≤ 0.5 mm

 

Unwinding tension with taper control (avoid constant tension that stretches the film)

 

Photoelectric edge guiding accuracy: ±0.3 mm; keep blades sharp (dull blades cause fibrilation and fuzzy edges)

 

Metering roller pressure: Light; excessive pressure causes bright streaks

 

Finished roll core hardness: Softer for household rolls, harder for industrial rolls — adjusted via rewinding taper

 

6. Essential Quality Inspections Before Shipment

 

Thickness: Target ±5% (premium lines achieve ±2 μm)

 

Self-adhesion: >0.3 N/25mm (peel test)

 

Haze / light transmittance: Low haze for high-clarity film

 

Tensile strength ≥20 MPa; elongation at break ≥200%

 

Pinholes: Zero pinholes per roll under light inspection

 

Migration, heavy metals, VCM: Third-party testing (SGS / CTI)

 

Roll length error: ±2%; edge misalignment ≤1 mm

 

7. Common Quality Issues & Solutions

latest company news about How to Produce High Quality Food Grade PVC Cling Film from our PVC Cling Film Machine  0 

 

In summary: High-quality PVC cling film = Low-migration DOTP/ATBC formulation + blown film multi-stage air cooling (or calendering with roll temp. difference ≤2°C) + constant-tension static-free winding + matched taper tension on rewinding machine. If the jumbo roll quality is poor, even the most expensive rewinder cannot fix the hand feel.